Amstrong® advanced high strength steels are available as thermomechanically hot rolled and cold formable grades.
Technical information
Amstrong®'s main properties include high yield strength and tensile strength combined with excellent formability, toughness at low temperatures, and fatigue resistance. These grades are therefore an excellent choice for reducing thickness and weight whilst improving load-bearing capacity, thereby generating cost savings and securing market advantage.
These grades also have better ductility and bendability than standard high strength low alloy (HSLA) grades. They are therefore perfect for demanding processes, resulting in trouble‑free operations and ensuring constant properties from one batch of material to the next. This results in a better yield on the production line and helps to achieve the most severe tolerances on the finished steel parts. With low P and Si content, the chemical composition of these grades makes them suitable for hot dip galvanising. Compared with the requirements of the EN 10149‑2 standard, all products come with a toughness guarantee of 40 J minimum at ‑20 °C (1) and mechanical properties guaranteed in the rolling and transverse directions.
Mechanical properties
| Grade | Direction | Thickness (mm) | Re (MPa) | Rm (MPa) | A80 (%) | A 5.65√So (%) | Min. mandrel diameter for 180° bending |
KV -20°C (J) |
|---|---|---|---|---|---|---|---|---|
| Amstrong® 240MC | L | < 3 | 240 - 320 | 340 - 450 | ≥ 27 | - | 0 | - |
| 3 - 6 | - | ≥ 32 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 260 - 340 | 340 - 450 | ≥ 26 | ≥ 31 | - | - | |
| 3 - 16 | - | - | ||||||
| Amstrong® 280MC | L | < 3 | 280 - 350 | 370 - 450 | ≥ 26 | - | - | - |
| 3 - 6 | - | ≥ 30 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 300 - 380 | 370 - 450 | ≥ 25 | - | 0 | - | |
| 3 - 16 | - | ≥ 29 | ||||||
| Amstrong® 315MC | L | < 3 | 315 - 395 | 415 - 495 | ≥ 24 | - | - | - |
| 3 - 6 | - | ≥ 28 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 340 - 420 | 420 - 500 | ≥ 23 | - | 0 | - | |
| 3 - 16 | - | ≥ 27 | ||||||
| Amstrong® 355MC | L | < 3 | 355 - 435 | 430 - 520 | ≥ 22 | - | - | - |
| 3 - 6 | - | ≥ 25 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 380 - 460 | 440 - 530 | ≥ 21 | - | 0 | - | |
| 3 - 16 | - | ≥ 24 | ||||||
| Amstrong® 390MC | L | < 3 | 390 - 480 | 460 - 560 | ≥ 20 | - | - | - |
| 3 - 6 | - | ≥ 24 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 420 - 500 | 470 - 570 | ≥ 19 | - | 0 | - | |
| 3 - 16 | - | ≥ 23 | ||||||
| Amstrong® 420MC | L | < 3 | 420 - 520 | 490 - 600 | ≥ 18 | - | - | - |
| 3 - 6 | - | ≥ 22 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 450 - 550 | 500 - 600 | ≥ 17 | - | ≥ 0.2 x t | - | |
| 3 - 16 | - | ≥ 21 | ||||||
| 13 - 16 | ≥ 0.5 x t | |||||||
| Amstrong® 460MC | L | < 3 | 460 - 560 | 520 - 640 | ≥ 15 | - | - | - |
| 3 - 6 | - | ≥ 18 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 490 - 590 | 530 - 640 | ≥ 14 | - | ≥ 0.6 x t | - | |
| 3 - 6 | - | ≥ 17 | ||||||
| 6 - 16 | ≥ 1 x t | |||||||
| Amstrong® 500MC | L | < 2 | 500 - 600 | 560 - 700 | ≥ 15 | - | - | - |
| 2 - 3 | ≥ 16 | |||||||
| 3 - 6 | - | ≥ 19 | ||||||
| 6 - 16 | - | ≥ 40 | ||||||
| T | < 2 | 530 - 630 | 570 - 700 | ≥ 14 | - | ≥ 0.6 x t | - | |
| 2 - 3 | ≥ 15 | |||||||
| 3 - 6 | - | ≥ 18 | ||||||
| 6 - 16 | - | ≥ 1 x t | ||||||
| Amstrong® 550MC | L | < 3 | 550 - 650 | 620 - 750 | ≥ 12 | - | - | - |
| 3 - 6 | - | ≥ 14 | ||||||
| 6 - 16 | ≥ 40 | |||||||
| T | < 3 | 580 - 680 | 630 - 750 | ≥ 11 | - | ≥ 0.8 x t | - | |
| 3 - 6 | - | ≥ 13 | ||||||
| 6 - 16 | ≥ 1.5 x t | |||||||
| Amstrong® 600MC | L | 2 - 3 | ≥ 600 | 650 - 820 | ≥ 11 | - | - | - |
| 3 - 6 | - | ≥ 13 | ||||||
| 6 - 10 | ≥ 40 | |||||||
| T | 2 - 3 | ≥ 620 | 660 - 820 | ≥ 10 | - | ≥ 1.5 x t | - | |
| 3 - 10 | - | ≥ 12 |
1) Grades in italics: not included in the standard
2) Values in bold: tighter than the standard
3) For Amstrong® grades, the mechanical properties are guaranteed in both directions.
4) Minimum specified mandrel diameter for bending angles up to 180° according to EN 10149-2:2013
5) t = nominal thickness
6) Toughness guarantee at -40°C: on request
Chemical properties
| Grade | C (%) |
Mn (%) |
P (%) |
S (%) |
Si (%) |
Al (%) |
Nb (%) |
V (%) |
Ti (%) |
Ceq (%) |
Mo (%) | B (%) |
Galvanisation |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Amstrong® 240MC | ≤ 0.100 | ≤ 0.80 | ≤ 0.020 | ≤ 0.020 | ≤ 0.03 | ≥ 0.015 | ≤ 0.025 | ≤ 0.200 | ≤ 0.150 | ≤ 0.18 | - | - | Class 1 |
| Amstrong® 280MC | ≤ 0.080 | ≤ 0.80 | ≤ 0.020 | ≤ 0.015 | ≤ 0.03 | ≥ 0.015 | ≤ 0.025 | ≤ 0.200 | ≤ 0.150 | ≤ 0.23 | - | - | Class 1 |
| Amstrong® 315MC | ≤ 0.100 | ≤ 0.70 | ≤ 0.020 | ≤ 0.015 | ≤ 0.03 | ≥ 0.015 | ≤ 0.045 | ≤ 0.200 | ≤ 0.150 | ≤ 0.25 | - | - | Class 1 |
| Amstrong® 355MC | ≤ 0.100 | ≤ 1.40 | ≤ 0.020 | ≤ 0.015 | ≤ 0.03 | ≥ 0.015 | ≤ 0.065 | ≤ 0.200 | ≤ 0.150 | ≤ 0.32 | - | - | Class 1 |
| Amstrong® 390MC | ≤ 0.100 | ≤ 1.50 | ≤ 0.020 | ≤ 0.012 | ≤ 0.03 | ≥ 0.015 | ≤ 0.065 | ≤ 0.200 | ≤ 0.150 | ≤ 0.36 | - | - | Class 1 |
| Amstrong® 420MC | ≤ 0.110 | ≤ 1.50 | ≤ 0.020 | ≤ 0.012 | ≤ 0.03 | ≥ 0.015 | ≤ 0.065 | ≤ 0.200 | ≤ 0.150 | ≤ 0.38 | - | - | Class 1 |
| Amstrong® 460MC | ≤ 0.120 | ≤ 1.50 | ≤ 0.020 | ≤ 0.012 | ≤ 0.03 | ≥ 0.015 | ≤ 0.080 | ≤ 0.200 | ≤ 0.150 | ≤ 0.40 | - | - | Class 1 |
| Amstrong® 500MC | ≤ 0.120 | ≤ 1.70 | ≤ 0.020 | ≤ 0.012 | ≤ 0.03 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | ≤ 0.42 | - | - | Class 1 |
| Amstrong® 550MC | ≤ 0.100 | ≤ 1.70 | ≤ 0.020 | ≤ 0.012 | ≤ 0.03 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | ≤ 0.44 | - | - | Class 1 |
| Amstrong® 600MC | ≤ 0.120 | ≤ 1.90 | ≤ 0.020 | ≤ 0.015 | ≤ 0.03 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.220 | ≤ 0.44 | ≤ 0.50 | ≤ 0.0050 | Class 1 |
1) Grades in italics: not included in the standard
2) Values in bold: tighter than the standard
3) The chemical properties given are based on cast analysis data.
4) V+Nb+Ti ≤ 0.22%
5) Suitability for hot dip zinc coating is defined as per the requirements of EN ISO 14713-2 Table 1 and NFA 35-503.