Steel grades for flat products made of weldable, hot rolled, high yield strength alloy quality and special steels for cold forming.
Thickness ranges from 1.5 to 20mm depending on the grade.
Technical information
Product definitions are produced in accordance with the EN10149 standard and concern hot rolled flat products made of high yield strength steels for cold forming.
EN10149 - 2 describes technical delivery conditions for thermomechanical rolled steels.
Mechanical properties
| EN standard | Grade | Direction | Thickness (mm) | Re (MPa) | Rm (MPa) | A80 (%) | A 5.65√So (%) | Min. mandrel diameter for 180° bending |
KV -20°C (J) |
|---|---|---|---|---|---|---|---|---|---|
| EN 10149-2 | S315MC | L | 1.5 - 3 | ≥ 315 | 390 - 510 | ≥ 20 | - | - | - |
| 3 - 20 | - | ≥ 24 | |||||||
| T | 1.5 - 20 | - | - | - | - | 0 | - | ||
| EN 10149-2 | S355MC | L | 1.5 - 3 | ≥ 355 | 430 - 550 | ≥ 19 | - | - | - |
| 3 - 20 | - | ≥ 23 | |||||||
| T | 1.5 - 20 | - | - | - | - | ≥ 0.5 x t | - | ||
| EN 10149-2 | S420MC | L | 1.5 - 3 | ≥ 420 | 480 - 620 | ≥ 16 | - | - | - |
| 3 - 20 | - | ≥ 19 | |||||||
| T | 1.5 - 20 | - | - | - | - | ≥ 0.5 x t | - | ||
| EN 10149-2 | S460MC | L | 1.5 - 3 | ≥ 460 | 520 - 670 | ≥ 14 | - | - | - |
| 3 - 16 | - | ≥ 17 | |||||||
| T | 1.5 - 20 | - | - | - | - | ≥ 1 x t | - | ||
| EN 10149-2 | S500MC | L | 1.5 - 3 | ≥ 500 | 550 - 700 | ≥ 12 | - | - | - |
| 3 - 16 | - | ≥ 14 | |||||||
| 16 - 20 | - | ||||||||
| T | 1.5 - 16 | - | - | - | - | ≥ 1 x t | - | ||
| EN 10149-2 | S550MC | L | 1.5 - 3 | ≥ 550 | 600 - 760 | ≥ 12 | - | - | - |
| 3 - 16 | - | ≥ 14 | |||||||
| 16 - 20 | - | ||||||||
| T | 1.5 - 16 | - | - | - | - | ≥ 1.5 x t | - | ||
| EN 10149-2 | S600MC | L | 2 - 3 | ≥ 600 | 650 - 820 | ≥ 11 | - | - | - |
| 3 - 10 | - | ≥ 13 | |||||||
| T | 2 - 10 | - | - | - | - | ≥ 1.5 x t | - | ||
| EN 10149-2 | S650MC | L | 2- 3 | ≥ 650 | 700 - 880 | ≥ 10 | - | - | - |
| 3 - 8 | - | ≥ 12 | |||||||
| 8 - 10 | ≥ 630 | ||||||||
| T | 2 - 10 | - | - | - | - | ≥ 2 x t | - | ||
| EN 10149-2 | S700MC | L | 2 - 3 | ≥ 700 | 750 - 950 | ≥ 10 | - | - | - |
| 3 - 8 | - | ≥ 12 | |||||||
| 8 - 10 | ≥ 680 | ||||||||
| T | 2 - 10 | - | - | - | - | ≥ 2 x t | - |
1) Minimum specified mandrel diameter for bending angles up to 180° according to EN 10149-2:2013
2) t = nominal thickness
3) Toughness guarantee at -40°C: on request
Chemical properties
| EN standard | Grade | C (%) |
Mn (%) |
P (%) |
S (%) |
Si (%) |
Al (%) |
Nb (%) |
V (%) |
Ti (%) |
Ceq (%) |
Mo (%) | B (%) |
Galvanisation |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| EN 10149-2 | S315MC | ≤ 0.120 | ≤ 1.30 | ≤ 0.025 | ≤ 0.020 | ≤ 0.50 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | - | - | - | No |
| EN 10149-2 | S355MC | ≤ 0.120 | ≤ 1.50 | ≤ 0.025 | ≤ 0.020 | ≤ 0.50 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | - | - | - | No |
| EN 10149-2 | S420MC | ≤ 0.120 | ≤ 1.60 | ≤ 0.025 | ≤ 0.015 | ≤ 0.50 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | - | - | - | No |
| EN 10149-2 | S460MC | ≤ 0.120 | ≤ 1.60 | ≤ 0.025 | ≤ 0.015 | ≤ 0.50 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | - | - | - | No |
| EN 10149-2 | S500MC | ≤ 0.120 | ≤ 1.70 | ≤ 0.025 | ≤ 0.015 | ≤ 0.50 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | - | - | - | No |
| EN 10149-2 | S550MC | ≤ 0.120 | ≤ 1.80 | ≤ 0.025 | ≤ 0.015 | ≤ 0.50 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.150 | - | - | - | No |
| EN 10149-2 | S600MC | ≤ 0.120 | ≤ 1.90 | ≤ 0.025 | ≤ 0.015 | ≤ 0.50 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.220 | - | ≤ 0.50 | ≤ 0.0050 | No |
| EN 10149-2 | S650MC | ≤ 0.120 | ≤ 2.00 | ≤ 0.025 | ≤ 0.015 | ≤ 0.60 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.220 | - | ≤ 0.50 | ≤ 0.0050 | No |
| EN 10149-2 | S700MC | ≤ 0.120 | ≤ 2.10 | ≤ 0.025 | ≤ 0.015 | ≤ 0.60 | ≥ 0.015 | ≤ 0.090 | ≤ 0.200 | ≤ 0.220 | - | ≤ 0.50 | ≤ 0.0050 | No |
1) The chemical properties given are based on cast analysis data.
2) V+Nb+Ti ≤ 0.22%
3) Suitability for hot dip zinc coating is defined as per the requirements of EN ISO 14713-2 Table 1 and NFA 35-503.